ROOF-210 · Lesson 5 of 12 · 25 min

Modified bitumen: SBS and APP

▶ Video coming soon A video version of this lesson is on the way.

Crew 2's next job, starting Monday, November 9, was a full re-roof on the Carrick Street building, a two-storey office built in 1996 with a dental clinic, an accountant and a physiotherapy practice as tenants. The old roof was a single ply of smooth-surfaced APP modified bitumen, torch-applied over fibreboard on a steel deck. Thirty years of sun had crazed its surface into a pattern of fine cracks, several laps had opened, and the property manager, Celeste Ward, had a bucket under a ceiling tile in the physiotherapy waiting room. The new roof, specified by a roof consultant, was a two-ply SBS system: a self-adhered base sheet and a torch-applied granulated cap sheet, with flameless details at the perimeter and penetrations.

On Friday afternoon, November 6, back at the yard after the Ferncliff repair, Rory helped Dana check the delivery. "Same family of material, completely different animals," she said, tapping a roll of the old APP sheet the consultant had sent for comparison and then a new SBS cap. "Bend that one at this temperature and it cracks. Bend this one and it just bends." This lesson explains what modified bitumen is, how SBS and APP differ, how the sheets are built and classified, and how a two-ply roof is laid out and estimated.

What modified bitumen is

Modified bitumen is asphalt blended in the factory with a polymer that changes how it behaves, then formed into sheets around a reinforcing mat. Plain roofing asphalt is stiff and brittle in the cold and soft in the heat. Adding polymer widens the temperature range over which the bitumen stays flexible and strong. The factory controls the polymer content, the thickness of bitumen on each side of the mat and the surfacing, so every square metre of sheet is the same.

Two polymers dominate:

  • SBS (styrene-butadiene-styrene) is a synthetic rubber. It makes the bitumen elastomeric: it stretches and recovers like rubber, and it stays flexible in cold weather.
  • APP (atactic polypropylene) is a plastic. It makes the bitumen plastomeric: stiffer and tougher, with good resistance to high temperatures and to sunlight, but less flexible in the cold.
Cut-away of a modified bitumen cap sheet: mineral granules on top, a layer of modified bitumen, the reinforcing mat in the middle, another layer of bitumen, and a backing of sand or burn-off film. A granule-free selvage strip runs along one edge for the side lap. Below, a comparison of SBS (rubber-like, stretches and recovers, flexible in the cold) and APP (plastic-like, stiffer, resists heat and sunlight).
How a modified bitumen sheet is built, and how SBS and APP differ.

SBS and APP compared

SBS and APP modified bitumen compared (typical values; check the product data sheet).
PropertySBSAPP
Natureelastomeric (rubber-like)plastomeric (plastic-like)
Cold-weather flexibilitytypically flexible to about −18 to −25 °C (0 to −13 °F)typically stiff near freezing or a few degrees below
Heat resistancegoodvery good; does not flow until much hotter
Sunlightmust be surfaced (granules or coating)better resistance; some APP sheets were sold smooth, but most are surfaced today
Installation methodstorch, hot asphalt, cold adhesive, self-adheredmostly torch or heat-welded; some cold-adhered
Hot asphaltbonds well when moppednot usually mopped; hot asphalt does not bond well to most APP
Where it is commoncold climates, including most of Canada and the northern UShot, sunny climates; some repairs and older roofs in the north

For a roof in Hamilton, where winter nights drop well below freezing and the roof surface swings 60 °C (110 °F) or more between a January night and a July afternoon, SBS is the usual choice, and nearly all of Ridgecap's mod-bit work is SBS. The old APP roof on Carrick Street was not wrong when it was built, but it is a reminder that an APP sheet that sat in a cold truck can crack if it is bent too sharply, and that repairs to an old APP roof need APP-compatible materials.

Reinforcement

The mat in the middle of the sheet carries tension and holds the bitumen in place. The main types:

  • Polyester: a non-woven polyester fabric. It stretches a long way before tearing, resists punctures and survives building movement and repeated foot traffic. It is the usual reinforcement for cap sheets and heavy-duty base sheets.
  • Glass fibre: a glass mat. It is very stable, so the sheet does not shrink or grow with temperature, but it stretches little and can tear more easily if the building moves. It is common in base sheets.
  • Composite: polyester and glass combined, for stability and strength together.

The reinforcement also decides how the sheet should be handled. A glass-mat sheet folded sharply in cold weather can crack the mat. A polyester sheet can stretch out of shape if it is pulled hard while hot from the torch.

Surfaces and edges

  • Mineral granules on the top of cap sheets protect the bitumen from sunlight, add fire resistance and come in colours, including white for reflectivity.
  • Sand or a fine mineral on base sheets and the underside of many sheets stops the roll sticking to itself and gives a surface that bonds to adhesive or hot asphalt.
  • A thin plastic burn-off film on the underside of torch-grade sheets stops the roll sticking. The torch shrinks and burns it away as the sheet is laid; a visible change in the film's pattern tells the applicator the bitumen is ready.
  • A release film or paper protects the adhesive side of self-adhered sheets (lesson 7).
  • A selvage edge is a granule-free strip, about 75 to 100 mm (3 to 4 in) wide, along one side of a cap sheet. The next sheet laps onto it, so bitumen bonds to bitumen rather than to granules.

Standards and how sheets are classified

In Canada, modified bitumen sheets are classified under CSA A123.23. The standard groups sheets by Type, the reinforcement (A glass fibre, B polyester, C composite), and by Grade, the surfacing and exposure (1 mineral granules, 2 other sun protection or unsurfaced, 3 not intended to be exposed, as for base sheets). A cap sheet listed as B1, for example, is polyester-reinforced and granule-surfaced. US projects use the ASTM standards: D6162, D6163 and D6164 for SBS sheets with composite, glass and polyester reinforcement, and D6222, D6223 and D6509 for APP sheets.

A specification usually names a product, or lists the standard, type and grade it must meet. Before a delivery goes up on the roof, check the roll labels against the specification: the product name, the standard, and the lot numbers, which the manufacturer's warranty inspector may ask for.

A two-ply system

Most new mod-bit roofs are two-ply: a base sheet and a cap sheet. The base gives the second line of waterproofing and a smooth surface for the cap; the cap carries the surfacing. Some specifications add an interply, making three plies, or use BUR plies under a mod-bit cap (a hybrid). The usual layout rules:

  • Start at the low point of the roof and lay sheets so that laps run with the water. On most low-slope roofs, sheets run parallel to the low edge or the drain line.
  • Side laps of at least 75 mm (3 in) and end laps of at least 150 mm (6 in), or as the maker requires.
  • Stagger end laps in adjacent sheets by at least 900 mm (3 ft).
  • Offset the cap sheet's side laps from the base sheet's side laps, so they never lie on top of each other. Many makers ask for about half a sheet width; Ridgecap's standard offset is 450 mm (18 in).
  • Cut the corner of the end-lap sheet at a T-joint, where an end lap crosses a side lap, about 75 mm (3 in) on the diagonal, so there is no open channel.
  • On steeper slopes, the maker may require sheets to run up the slope and be fastened at the top (back-nailed) to stop them sliding.
Plan of a two-ply modified bitumen layout from the low edge: base sheets with 75 mm side laps, cap sheets offset 450 mm so their laps fall between the base laps, end laps 150 mm staggered at least 900 mm, and a T-joint with the corner cut at 75 mm.
Laying out a two-ply modified bitumen roof.

Rolls and quantities

Rolls are sold by gross area, but the laps use some of every roll. The net coverage is what counts.

Worked problem

Net coverage of a cap roll

A cap roll is 1.0 m wide and 8.0 m long. Side laps are 75 mm and end laps 150 mm. What area does one roll cover once lapped?

Show solution
  1. Effective width = 1.000 − 0.075 = 0.925 m.
  2. Effective length = 8.00 − 0.15 = 7.85 m.
  3. Net area = 0.925 × 7.85 = 7.26 m².
  4. Gross area is 8.0 m², so laps use 8.0 − 7.26 = 0.74 m², about 9 per cent.

Answer: Each cap roll covers about 7.26 m² of roof.

Worked problem

Rolls for Carrick Street

The Carrick Street roof is 38.0 m by 20.0 m. Base rolls are 1.0 m by 20.0 m and cap rolls 1.0 m by 8.0 m, with the same laps. Add 5 per cent for cutting waste. Flashings are counted separately. How many rolls of each?

Show solution
  1. Roof area = 38.0 × 20.0 = 760 m².
  2. Base net per roll = 0.925 × (20.0 − 0.15) = 0.925 × 19.85 = 18.36 m².
  3. Base rolls = 760 ÷ 18.36 × 1.05 = 43.5, so 44 rolls.
  4. Cap net per roll = 7.26 m²; cap rolls = 760 ÷ 7.26 × 1.05 = 109.9, so 110 rolls.

Answer: 44 base rolls and 110 cap rolls for the field, before flashings.

The two sites' cap counts differ because the cap rolls are different sizes, 8 m² gross in this example. Always figure from the roll actually being bought.

Storing and loading rolls

Modified bitumen rolls are heavy and easy to damage:

  • Store rolls on end, on pallets, off the ground. A roll stored on its side flattens, and a flat roll lays out with a permanent wrinkle or dog-leg.
  • Cover them with breathable tarps, not plastic, which traps moisture. Keep self-adhered rolls out of direct sun, which can soften the adhesive layer.
  • In cold weather, keep the day's rolls warm, at about 10 °C (50 °F) or more for 24 hours before use, as lesson 4 described.
  • Do not drop rolls or throw them off the hoist. A dented roll edge makes a crooked lap.
  • Spread pallets over the roof structure. The roof must be able to carry the load, and a full pallet is a concentrated load.

Worked problem

A pallet on the roof

A 4 mm SBS cap weighs about 4.6 kg/m². A pallet holds 25 rolls of 8.0 m² each, plus 20 kg of pallet. What is the load, and what is it per square metre if the pallet is 1.1 m by 1.1 m?

Show solution
  1. One roll = 8.0 × 4.6 = 36.8 kg.
  2. Pallet load = 25 × 36.8 + 20 = 940 kg.
  3. Footprint = 1.1 × 1.1 = 1.21 m².
  4. Pressure = 940 ÷ 1.21 = 777 kg/m², about 7.6 kPa.

Answer: Nearly a tonne on 1.21 m², several times a typical roof design load. Dana has the hoist operator set pallets directly over the steel joists near the columns and spread rolls out within the hour.

Reading the old roof

When the crew cut the first test opening on Carrick Street on Monday morning, Rory could see everything the lesson had described. The old APP sheet's smooth surface was crazed and chalky. Its laps were bonded where the torch had heated them well and open where it had not. Under it, the fibreboard was soft and dark near the physiotherapy leak. The new two-ply SBS system would go over a new cover board on new insulation, with granules to protect it from the sun the old sheet had had to face bare.

Reading a roll label

Every roll carries a label or wrapper printed with the information the crew and the inspector need. Rory copied the one from a Carrick Street cap into his notebook:

  • Product name and type: base or cap, SBS or APP, and the installation method it is made for, such as torch, cold adhesive, hot asphalt or self-adhered.
  • The standard it meets: CSA A123.23 type and grade, and often the ASTM number as well.
  • Thickness or weight, roll width and length, and gross coverage.
  • Lot or batch number and date of manufacture.
  • Storage and handling instructions: store on end, protect from moisture and sun, and the minimum temperatures for application.

Mixing products with different installation methods is a common error on busy jobs. A cold-adhesive cap torched by mistake, or a torch cap set in cold adhesive, may bond poorly and is not covered by the warranty. Dana's rule: read the label of every pallet as it comes off the hoist, and keep different products in separate, marked stacks.

Repairing an old APP roof

Ridgecap still repairs APP roofs from the 1990s and 2000s. Repairs use APP-compatible materials, usually a torch-grade APP or a maker-approved repair sheet, after the surface is cleaned and primed. Old APP is stiff in the cold, so repairs are planned for warm weather where possible, and patches are heated gently so the old sheet does not crack as it is bent.

Common mistakes

  • MistakeTreating SBS and APP as the same.

    InsteadSBS is elastomeric and flexible in the cold; APP is plastomeric, stiffer and usually torch-applied. Match repairs to the existing sheet.

  • MistakeLining up cap laps over base laps.

    InsteadOffset cap side laps from base side laps, about 450 mm (18 in) at Ridgecap.

  • MistakeCounting rolls from gross area.

    InsteadUse net coverage after side and end laps, then add waste.

  • MistakeStoring rolls on their sides.

    InsteadStore on end, on pallets, under breathable covers; keep them warm in cold weather.

  • MistakeLeaving full pallets in one spot on the roof.

    InsteadSet pallets over structure and spread the load quickly.

Summary and key terms

  • Modified bitumen is asphalt blended with SBS or APP polymer and formed around a reinforcing mat in the factory.
  • SBS is rubber-like and flexible in the cold; APP is plastic-like, stiffer and resistant to heat and sunlight.
  • Polyester reinforcement stretches and resists punctures; glass is stable; composite combines them.
  • CSA A123.23 classifies sheets by reinforcement type and surfacing grade; ASTM D6162 to D6164 and D6222, D6223 and D6509 cover SBS and APP sheets.
  • A two-ply roof has side laps of 75 mm (3 in), end laps of 150 mm (6 in) staggered 900 mm (3 ft), and cap laps offset from base laps.
  • Figure rolls from net coverage, and store and load rolls so they stay round, warm and spread out.
Modified bitumen
Asphalt modified with a polymer such as SBS or APP and made into reinforced roofing sheets.
SBS
Styrene-butadiene-styrene, a rubber polymer that makes bitumen elastomeric and flexible in the cold.
APP
Atactic polypropylene, a plastic polymer that makes bitumen stiffer and resistant to heat.
Reinforcement
The polyester, glass or composite mat inside a modified bitumen sheet.
Selvage edge
A granule-free strip along the edge of a cap sheet where the next sheet laps.
Burn-off film
A thin plastic film on torch-grade sheets that the torch melts away during application.
Base sheet
The bottom ply of a multi-ply modified bitumen roof.
Cap sheet
The top, surfaced ply of a modified bitumen roof.

Practice problems

Work each problem on paper first, then reveal the answer to check.

  1. A base roll is 1.0 m by 15.0 m with 75 mm side and 150 mm end laps. What is its net coverage?

    Show answer

    0.925 × 14.85 = 13.74 m².

  2. How many 7.26 m² net cap rolls cover 500 m² with 5 per cent waste?

    Show answer

    500 ÷ 7.26 × 1.05 = 72.3, so 73 rolls.

  3. What does Grade 1 mean under CSA A123.23?

    Show answer

    The sheet is surfaced with mineral granules.

  4. Why are cap side laps offset from base side laps?

    Show answer

    So the laps never lie on top of each other and form a weak line through both plies.

  5. Which polymer would you choose for a cold-climate roof that will be mopped in hot asphalt?

    Show answer

    SBS.

Lesson quiz · 5 questions

Score 60% or more to complete this lesson.

Take the quiz